Difference between revisions of "CiM"

From Fritipedia
Jump to navigationJump to search
 
(33 intermediate revisions by 2 users not shown)
Line 1: Line 1:
 
CIM stands for Creation Is Messy. They are suppliers of [[glass]] which hs a [[CoE]] of 104 and is compatible with [[Effetre]], [[Vetrofond]], [[Lauscha]] and the other 104 glasses. The messy colour pallettes are being extended regularly with new shades. They also produce a range of [[CoE]] 96 glass called Messy 96. Messy colour 104 and Messy 96 are not [[compatible]].  
 
CIM stands for Creation Is Messy. They are suppliers of [[glass]] which hs a [[CoE]] of 104 and is compatible with [[Effetre]], [[Vetrofond]], [[Lauscha]] and the other 104 glasses. The messy colour pallettes are being extended regularly with new shades. They also produce a range of [[CoE]] 96 glass called Messy 96. Messy colour 104 and Messy 96 are not [[compatible]].  
  
Occasionally CiM produce a pull of glass that does conform exactly to their colour specifications or one that is created for a test run. These occasional odd lots of glass are labled as "Messy Uniques" and are sold exclusively by Frantz art glass and associated sellers in the U.S.A.
+
Occasionally CiM produce a pull of glass that does not conform exactly to their colour specifications or one that is created for a test run. These occasional odd lots of glass are labled as "Messy Uniques."  
  
 
==Creation in Messy 104 colours and stock numbers==
 
==Creation in Messy 104 colours and stock numbers==
  
  
Information on the working properties of CiM glass is a current research project by members of the Frit-Happens community in the form of a prize competition  
+
Information on the working properties of CiM glass is a research project by members of the Frit-Happens community in the form of a prize competition  
[http://www.frit-happens.co.uk/forum/index.php?topic=9536.0 Frit-Happens CiM Competition Thread]  
+
[http://www.frit-happens.co.uk/forum/index.php?topic=9536.0 Frit-Happens CiM Competition Thread] The information below has been collated by Jolene Wolfe [http://www.kitzbitzartglass.com kitzbitz art glass] and is intended as a guide only.
  
 
=== CiM 104 ===
 
=== CiM 104 ===
 +
Stock numbers are preceded with 511.
 
{| class="wikitable sortable" width=90%
 
{| class="wikitable sortable" width=90%
 
|-
 
|-
Line 18: Line 19:
 
! Reactions
 
! Reactions
 
|-
 
|-
|C0109
+
|109
 
|bordello
 
|bordello
|annealing temp 504 degrees C
+
|  
|semi translucent deep red
+
|intense translucent deep red
 
|  
 
|  
 
|-
 
|-
|C0128
+
|128
 
|sangre
 
|sangre
 
|striking colour
 
|striking colour
 
|opaque red
 
|opaque red
|  
+
|no brown reaction with fine silver
 
|-
 
|-
|C0149
+
|149
 
|lipstick
 
|lipstick
 
|
 
|
|opaque red brown
+
|opaque red brown (brick)
 
|  
 
|  
 
|-
 
|-
|C0223
+
|223
 
|pumpkin
 
|pumpkin
 
|
 
|
Line 42: Line 43:
 
|  
 
|  
 
|-
 
|-
|C0229
+
|229
 
|clockwork
 
|clockwork
|
+
|intense striking colour - stiff glass
|opaque deep orange
+
|deep orange
|
+
|becomes more opaque in a reduction flame
 
|-
 
|-
|C0241
+
|241
 
|creamsicle
 
|creamsicle
 +
|not a spreading colour
 +
|opaque orange
 
|
 
|
|semi opaque orange
+
|-
 +
|277
 +
|phoenix
 +
|striking colour
 +
|Orange
 
|
 
|
 
|-
 
|-
|C0346
+
|346
 
|ghee
 
|ghee
|
+
|strikes from light yellow to shades of caramel
 
|semi opaque light yellow
 
|semi opaque light yellow
 
|  
 
|  
 
|-
 
|-
|C0351
+
|351
 
|stoneground
 
|stoneground
|
+
|works well in slightly reducing flame of a HH - reduction colour is orangy
 
|opaque light brown
 
|opaque light brown
|
+
|reacts with fine silver - reacts with ivory
 
|-
 
|-
|C0402
+
|402
|cedalon
+
|celadon
|annealing temp 554 degrees C
+
|not a spreading colour
 
|opaque turquoise
 
|opaque turquoise
|  
+
|reacts with ivory - little reaction with fine silver
 
|-
 
|-
|C0413
+
|413
 
|peacock green
 
|peacock green
|annealing temp 538 degrees C - shocky - anneal from hot
+
|shocky - anneal from hot - works well in slightly reducing flame of a HH
|semi translucent light green
+
|translucent light green
 
|
 
|
 
|-
 
|-
|C0430
+
|430
 
|elphaba
 
|elphaba
|
+
|not a spreading colour - reduces to brown tones - Can appear striated
 
|opaque light green
 
|opaque light green
 
|
 
|
 
|-
 
|-
|C0448
+
|448
 
|dirty martini
 
|dirty martini
 +
|perfectly complimented by [[Reichenbach]] antique clear
 +
|opaque pale green
 +
|lace reaction with nero intenso - fumed easily by by silver glass and SiS and reacts butifully with fine silver leaf
 +
|-
 +
|449
 +
|kryptonite
 +
|striking - does not work well in slightly reducing flame of a HH
 +
|semi opaque light green
 +
|does not react strongly with silver glass
 +
|-
 +
|475
 +
|commando
 +
|
 +
|opaque green
 +
|
 +
|-
 +
|476
 +
|olive
 +
|
 +
|opaque green
 +
|
 +
|-
 +
|478
 +
|oz
 +
|
 +
|vibrant trans green
 +
|
 +
|-
 +
|479
 +
|soylent
 +
|
 +
|opaque green
 +
|
 +
|-
 +
|481
 +
|splitpea
 +
|heavy natural striations within this colour
 +
|opaque green
 +
|
 +
|-
 +
|482
 +
|mojito
 +
|
 +
|light trans green
 +
|
 +
|-
 +
|483
 +
|slytherin
 +
|very intensely saturated colour
 +
|dark trans green
 +
|
 +
|-
 +
|487
 +
|poison apple
 +
|
 +
|vibrant opal green
 +
|
 +
|-
 +
|492
 +
|sherwood
 +
|
 +
|opaque forest green
 +
|
 +
|-
 +
|497
 +
|appletini
 
|
 
|
|opaque pale green
+
|transparent bottle green
 +
|
 +
|-
 +
|499
 +
|rainforest
 +
|
 +
|greenish teal opal
 
|
 
|
 
|-
 
|-
|C0449
+
|500
|kryptonite
+
|azure
 
|
 
|
|semi opaque light blue
+
|transparent blue
 
|
 
|
 
|-
 
|-
|C0505
+
|505
 
|french blue
 
|french blue
|
+
|has some striation
 
|opaque bright blue
 
|opaque bright blue
|
+
|etches beautifully - reacts with ivory
 
|-
 
|-
|C0508
+
|508
 
|leaky pen
 
|leaky pen
|annealing temp 527 degrees C - work high in flame as may pit
+
|Intense colour - work high in flame as may pit - works well in slightly reducing flame of a HH - spreading colour - takes on a metalic hue when reduced - stiff glass - takes longer to etch
 
|semi translucent dark blue
 
|semi translucent dark blue
|spreading colour
+
|looks black over rubiono oro
 
|-
 
|-
|C0512
+
|512
 
|halong bay
 
|halong bay
|annealing temp 549 degrees C - shocky - anneal from hot
+
|shocky - anneal from hot - works well in slightly reducing flame of a HH
|semi translucent light blue  
+
|opal light blue  
 
|
 
|
 
|-
 
|-
|C0519
+
|519
 
|glacier
 
|glacier
|
+
|light striations within this beautiful
 
|opaque light blue
 
|opaque light blue
 
|
 
|
 
|-
 
|-
|C0531
+
|531
 
|lapis
 
|lapis
 +
|works well in slightly reducing flame of a HH - reduces to a metalic sheen
 +
|dark opaque purple blue
 
|
 
|
|opaque purple blue
+
|-
 +
|543
 +
|sapphire
 +
|may pit if heated too quickly
 +
|transparent medium blue
 
|
 
|
 
|-
 
|-
|C0543
+
|547
|sapphire
+
|electric avenue
 +
|works well in slightly reducing flame of a HH
 +
|opal medium blue
 +
|brown reaction with fine silver - when heavily reduced goes deep terracotta - reacts with ivory
 +
|-
 +
|550
 +
|chalcedony
 +
|
 +
|opal light blue
 +
|has a light reaction with fine silver
 +
|-
 +
|562
 +
|ming
 
|
 
|
 +
|opal deep blue
 +
|coulour opacifies the longer it is worked
 +
|-
 +
|563
 +
|pulsar
 +
|may pit if heated too quickly
 
|transparent medium blue
 
|transparent medium blue
 +
|reacts with ivory
 +
|-
 +
|568
 +
|freman
 
|
 
|
 +
|opaque sky blue
 +
|reacts with silver - reacts with ivory
 
|-
 
|-
|C0547
+
|569
|electric avenue
+
|smurfy
 +
|
 +
|opaque turquoise
 +
|reacts with ivory
 +
|-
 +
|570
 +
|grumpy bear
 +
|some striation
 +
|opaque periwinkle
 +
|
 +
|-
 +
|571
 +
|cornflower
 +
|some striation
 +
|opaque periwinkle blue
 
|
 
|
|opaque medium blue
+
|-
 +
|586
 +
|mermaid
 +
|some striation
 +
|opaque teal
 
|
 
|
 
|-
 
|-
|C0550
+
|589
|chalcedony
+
|zachary
 
|
 
|
|opaque light blue
+
|opaque baby blue
 
|
 
|
 
|-
 
|-
|C0562
+
|590
|ming
+
|great bluedini
 
|
 
|
|opaque deep blue
+
|intense trasparent teal
 
|
 
|
 
|-
 
|-
|C0563
+
|598
|pulsar
+
|atlantis
 
|
 
|
|transparent medium blue
+
|bluish teal opal
 
|
 
|
 
|-
 
|-
|C0618
+
|618
 
|simply berry
 
|simply berry
|annealing temp 577 degrees C
+
|
 
|semi opaque light purple
 
|semi opaque light purple
|
+
|superheat with nero intenso stringer for "lace" effect - does not react as a base for silver glass
 
|-
 
|-
|C0632
+
|632
 
|thai orchid
 
|thai orchid
|
+
|intesne colour - some striation - works well in slightly reducing flame of a HH
 
|opaque violet
 
|opaque violet
|
+
|does not react with silver glass or SIS - spreads when superheated over a softer opaque base
 
|-
 
|-
|C0645
+
|645
 
|heffalump
 
|heffalump
|
+
|colour appears to "shift" in different lighting conditions - looks lovely coated with 00 lead crystal frit (sugared)
|opaque pale lilac
+
|opaque light lavender
|
+
|brown reaction with fine silver
 
|-
 
|-
|C0652
+
|652
 
|count von count
 
|count von count
|
+
|colour appears to "shift" in different lighting conditions
|transparent light purple
+
|transparent light purple/blue
 
|
 
|
 
|-
 
|-
|C0653
+
|653
 
|larkspur
 
|larkspur
|
+
|colour appears to "shift" in different lighting conditions
|transparent pale purple
+
|transparent pale purple/blue
|
+
|Does not lace with nero intenso
 
|-
 
|-
|C0654
+
|654
 
|grape ape
 
|grape ape
|
+
|works well in slightly reducing flame of a HH - some striation
 
|opaque medium purple
 
|opaque medium purple
|
+
|does not react with silver glass - reacts with [[Kugler 104 green]] - can "swallow" stringer - reacts with plum - reacts with copper colours
 
|-
 
|-
|C0655
+
|655
 
|eggplant
 
|eggplant
|
+
|saturated and intense - spreading colour - works well in slightly reducing flame of a HH - striking colour
 
|opaque dark purple
 
|opaque dark purple
 
|
 
|
 
|-
 
|-
|C0658
+
|658
 
|plum
 
|plum
|
+
|works well in slightly reducing flame of a HH - Looks beautiful encased in clear - spreading colour - striking colour
|semi translucent light purple
+
|opal light purple
|
+
|reacts with ivory - not fumed by gold leaf - can "swallow" stringer - reacts with grape ape - reacts with copper colours
 
|-
 
|-
|C0660
+
|660
 
|crocus
 
|crocus
|
+
|Looks beautiful encased in clear
 
|semi opaque light purple
 
|semi opaque light purple
 
|
 
|
 
|-
 
|-
|C0661
+
|661
 
|evil queen
 
|evil queen
 
|
 
|
Line 216: Line 343:
 
|
 
|
 
|-
 
|-
|C0667
+
|667
 
|poi
 
|poi
|
+
|some striation
|opaque dark lilac
+
|opaque dark lilac gray
 
|
 
|
 
|-
 
|-
|C0701
+
|701
 
|ginger
 
|ginger
|annealing temp 543 degrees C
+
|can be shocky
|opaque light pink
+
|opaque light neutral pink
|
+
|less reactive than ivory
 
|-
 
|-
|C0703
+
|703
 
|butter pecan
 
|butter pecan
|annealing temp 565 degrees C
+
|  
 
|opaque pale pink
 
|opaque pale pink
|
+
|less reactive than ivory - reacts with fine silver foil - reacts with celadon
 
|-
 
|-
|C0717
+
|717
 
|khaki
 
|khaki
|
+
|works well in slightly reducing flame of a HH
|opaque gray green
+
|opaque neutral gray  
|
+
|reacts with fine silver
 
|-
 
|-
|C0722
+
|722
 
|canyon de chelly
 
|canyon de chelly
|
+
|works well in slightly reducing flame of a HH - heavy striation - striking colour
|opaque light brown
+
|opaque silver light brown
|
+
|no lacing with nero intenso - looks great with raku
 
|-
 
|-
|C0742
+
|742
 
|sepia
 
|sepia
 +
|colour appears to "shift" in different lighting conditions - work cool
 +
|transparent pale pink/amber
 +
|Does not lace with nero intenso - no fuming with silver glass - very effective with SiS - look nice etched
 +
|-
 +
|780
 +
|maple
 
|
 
|
|transparent pale pink
+
|trans mid brown
 
|
 
|
 
|-
 
|-
|C0765
+
|788
|chai
+
|mink
 
|
 
|
|opaque pale pink
+
|opal chocolate browm
 
|
 
|
 
|-
 
|-
|C0806
+
|806
 
|cirrus
 
|cirrus
|annealing temp 521 degrees C - striking colour - shocky - anneal from hot
+
|striking colour - shocky - anneal from hot - does not etch - works well in slightly reducing flame of a HH
 
|semi opaque white  
 
|semi opaque white  
|reduces to yellow/brown
+
|reduces to yellow/brown - Dots of leaky Pen and Reichenbach gold violet "pool" when melted in to cirrus - becomes more opaque the longer you work it in the flame - can be fumed by silver
 
|-
 
|-
|C0820
+
|820
 
|hades
 
|hades
|
+
|dots crisp melted down over [[Effetre]] white - dots bleed into CiM peace - works well in slightly reducing flame of a HH
|opaque intense black
+
|opaque intense black - even as stringer
|
+
|reacts with ivory and opal yellow - laces as stringer over some base glasses including [[Effetre]] coral when superheated - fumes to irridescent green/blue with fine silver - reacts with palladium.
 
|-
 
|-
|C0834
+
|834
 
|clear
 
|clear
|
+
|work cool
 
|transparent clear
 
|transparent clear
 
|
 
|
 
|-
 
|-
|C0835
+
|835
 
|peace
 
|peace
 +
|saturated colour
 +
|shimmering opaque white
 
|
 
|
|shimmering opaque white
+
|-
 +
|859
 +
|marshmallow
 +
|Looks beautiful encased in clear
 +
|semi opaque white
 
|
 
|
 
|-
 
|-
|C0859
+
|872
|marshmallow
+
|tuxedo
 +
|
 +
|grey based opaque black
 +
|effetre white stringer breaks up organically over a tuxedo base
 +
|-
 +
|874
 +
|adamantium
 +
|
 +
|opaque dark grey
 
|
 
|
|semi opaque white
+
|-
 +
|885
 +
|gunmetal
 +
|soft glass
 +
|black glass that tends towards silver/pewter in a neutral to oxygen rich flame
 
|
 
|
 
|-
 
|-
|C0904
+
|904
 
|gelly's sty
 
|gelly's sty
|annealing temp 510 degrees C
+
|likes to be worked hot
 
|opaque  light pink
 
|opaque  light pink
 
|
 
|
 
|-
 
|-
|C0907
+
|907
 
|rose quartz
 
|rose quartz
 +
|likes to be worked hot (may devit in a cooler flame ) - looks lovely coated with 00 lead crystal frit (sugared)- striking colour
 +
|semi opaque light pink
 +
|brown reaction with fine silver
 +
|-
 +
|915
 +
|pink champagne
 +
|colour appears to "shift" in different lighting conditions
 +
|translucent light pink
 +
|brownish tint when used to encase white
 +
|-
 +
|921
 +
|blush
 +
|
 +
|trans pale pink
 +
|
 +
|-
 +
|926
 +
|cranberry pink
 +
|spreading colour - makes beautiful vivid pink when encased over white/dark fuchsia over ivory - burns less easily than Effetre Rubino Oro
 +
|semi opaque rich dark gold pink - available in two distinct shades (511926-1 light & 511926-2 dark)
 +
|very reactive (dirty martini, lapis)
 +
|-
 +
|957
 +
|desert pink
 +
|works well in slightly reducing flame of a HH
 +
|opaque pale pink
 +
|Fumed easily by silver glass
 +
|-
 +
|}
 +
 +
=== CiM Limited Runs ===
 +
 +
{| class="wikitable sortable" width=90%
 +
|-
 +
! width=50px|Stock Number
 +
! Colour
 +
! Properties
 +
! Other Info
 +
! Reactions
 +
|-
 +
|511484
 +
|algae
 +
|
 +
|transparent greyish green
 +
|
 +
|-
 +
|511656
 +
|black currant
 
|
 
|
|semi opaque light pink
+
|very dark purple (nearly black)
 +
|
 +
|-
 +
|511765
 +
|chai
 +
|
 +
|light opaque brown
 +
|
 +
|-
 +
|511773
 +
|tamarind
 +
|
 +
|opaque mid chocolate brown
 +
|
 +
|-
 +
|511795
 +
|adobe
 +
|
 +
|adobe brown opaque
 
|
 
|
 
|-
 
|-
|C0915
+
|511891
|pink champagne
+
|hippo
 
|
 
|
|translucent light pink
+
|opaque grey
 
|
 
|
 
|-
 
|-
|C0921
+
|511864
|blush
+
|charcoal
 +
|
 +
|very dark trans grey
 
|
 
|
|translucent pale pink
+
|-
 +
|511893
 +
|african gray
 +
|keeps cat's-eye sheen, good base for silver
 +
|opaque mid grey
 
|
 
|
 
|-
 
|-
|C0926
+
|511896
|cranberry
+
|oliphaunt
 +
|good base for silver
 +
|opaque grey, blueish not brown
 
|
 
|
|semi opaque rich dark pink
+
|-
 +
|511939 - cored cane
 +
|cranberry pink and gelly's sty
 +
|cored cane, heart shaped cranberry encased with gelly's sty
 +
|streaky pink when worked
 
|
 
|
 
|-
 
|-
|C0957
+
|511938 - cored cane
|desert pink
+
|peace and gelly's sty
 +
|cored cane, heart shaped peace encased with gelly's sty
 +
|streaky pink and red when worked
 +
|
 +
|-
 +
|511994
 +
|razzleberry
 
|
 
|
|opaque pale pink
+
|hot pink
 
|
 
|
 
|-
 
|-
 
|}
 
|}
  
 +
=== CiM Uniques ===
  
=== CiM Uniques ===
+
{| class="wikitable sortable" width=90%
 +
|-
 +
! width=50px|Stock Number
 +
! Colour
 +
! Properties
 +
! Other Info
 +
! Reactions
 +
|-
 +
|511128-1
 +
|sangre
 +
|
 +
|darker than regular sangre
 +
|
 +
|-
 +
|511140-1
 +
|lipstick
 +
|
 +
|lighter thank regular lipstick
 +
|
 +
|-
 +
|511140-3
 +
|lipstick
 +
|
 +
|lighter than 5111140-1
 +
|
 +
|-
 +
|511223-3
 +
|Pumpkin
 +
|not a spreading colour
 +
|lighter than regular pumpkin
 +
|
 +
|-
 +
|511223-3
 +
|pumpkin
 +
|
 +
|translucent burnt orange
 +
|
 +
|-
 +
|511333
 +
|sunshine
 +
|never went in to full production
 +
|soft buttery yellow
 +
|
 +
|-
 +
|511351-1
 +
|stone ground
 +
|
 +
|lighter than regular
 +
|
 +
|-
 +
|511413-2
 +
|peacock green
 +
|
 +
|slightly blueish compared to regular
 +
|
 +
|-
 +
|511413-3
 +
|peacock green
 +
|
 +
|more saturated than 511413-2
 +
|
 +
|-
 +
|511427
 +
|tabby gray
 +
|never went in to full production - looks great with SiS
 +
|silver gray
 +
|
 +
|-
 +
|511430-1
 +
|elphaba
 +
|
 +
|very similar to regular
 +
|
 +
|-
 +
|511430-2
 +
|elphaba
 +
|
 +
|petroleum green
 +
|
 +
|-
 +
|511430-3
 +
|elphaba
 +
|
 +
|darker than regular
 +
|
 +
|-
 +
|511449-1
 +
|kryptonite
 +
|
 +
|turns opaque more quickly than regular
 +
|
 +
|-
 +
|511531-1
 +
|lapis
 +
|
 +
|more purple than blue
 +
|
 +
|-
 +
|511618-1
 +
|simply berry
 +
|
 +
|lighter than regular
 +
|
 +
|-
 +
|511618-2
 +
|simply berry
 +
|
 +
|darker than regular
 +
|
 +
|-
 +
|511644
 +
|dusk
 +
|never went in to full production - colour shifts under different lighting
 +
|blue gray shade
 +
|looks a more neutral gray when used to encase white
 +
|-
 +
|511656
 +
|blackcurrant
 +
|almost black when used on its own
 +
|very dark purple
 +
|
 +
|-
 +
|511701-1
 +
|ginger
 +
|
 +
|lighter than regular
 +
|
 +
|-
 +
|511703-3
 +
|butter pecan
 +
|
 +
|darker than regular
 +
|
 +
|-
 +
|511703-3
 +
|butter pecan
 +
|
 +
|more yellow than regular
 +
|
 +
|-
 +
|511742-1
 +
|sepia
 +
|
 +
|more amber than regular
 +
|
 +
|-
 +
|511742-2
 +
|sepia
 +
|
 +
|melt came out blue
 +
|
 +
|-
 +
|511806-1
 +
|cirrus
 +
|striking colour
 +
|strikes to opaque more easily than regular
 +
|
 +
|-
 +
|511806-2
 +
|cirrus
 +
|striking colour
 +
|slight blue tint
 +
|
 +
|-
 +
|511904-1
 +
|gelly's sty
 +
|
 +
|less saturated than regular
 +
|
 +
|-
 +
|511957-1
 +
|desert pink
 +
|
 +
|brighter than regular
 +
|
 +
|-
 +
|511957-2
 +
|desert pink
 +
|
 +
|peachier / more brown than regular
 +
|
 +
|-
 +
|}
  
=== recommended batch annealing schedules for CiM ===
+
=== Two batch annealing schedules for CiM ===
  
 
525 (Celsius) annealing schedule for batch annealing
 
525 (Celsius) annealing schedule for batch annealing
  
Ramp up        0-150  degrees      1 hour     
+
Ramp up        0-150  degrees      1 hour     
 
                     150-315  degrees    1 hour   
 
                     150-315  degrees    1 hour   
 
                     315-425  degrees    1 hour   
 
                     315-425  degrees    1 hour   
 
                     425-525 degrees    1 hour
 
                     425-525 degrees    1 hour
 
                     Held at 525 for 30 minutes
 
                     Held at 525 for 30 minutes
Ramp down    525-425 degrees    2 hours
+
Ramp down    525-425 degrees    2 hours
 
                     425-370  degrees    1 hour  
 
                     425-370  degrees    1 hour  
 
                     370-315  degrees    1 hour
 
                     370-315  degrees    1 hour
 
                     315-205 degrees    1 hour
 
                     315-205 degrees    1 hour
                    Turn off kiln and remove beads the next morning.
+
Turn off kiln and remove beads the next morning.
  
 
555 (Celsius) annealing schedule for batch annealing
 
555 (Celsius) annealing schedule for batch annealing
  
Ramp up        0-150 degrees        1 hour
+
Ramp up        0-150 degrees        1 hour
 
                     150-315 degrees      1 hour  
 
                     150-315 degrees      1 hour  
 
                     315-425 degrees      45 minutes
 
                     315-425 degrees      45 minutes
Line 352: Line 770:
 
                     510-555  degrees    45 minutes
 
                     510-555  degrees    45 minutes
 
                     Held at 555 for 30 minutes
 
                     Held at 555 for 30 minutes
Ramp down    555-510 degrees      1 hour
+
Ramp down    555-510 degrees      1 hour
 
                     510-455 degrees      1 hour
 
                     510-455 degrees      1 hour
 
                     455-400 degrees      1 hour
 
                     455-400 degrees      1 hour
 
                     400-290 degrees      1 hour
 
                     400-290 degrees      1 hour
 
                     290-230 degrees      1 hour
 
                     290-230 degrees      1 hour
                    Turn off kiln and remove beads in the morning.
+
Turn off kiln and remove beads in the morning.
 
 
Information researched by CiM tester Lorraine Chandler
 
  
 +
Information researched by CiM tester [http://www.2toucanstreetopcreations.com/ Lorraine Chandler]
  
 
== Further information ==
 
== Further information ==
 
Visit their website for more information:
 
Visit their website for more information:
 
http://www.creationismessy.com/
 
http://www.creationismessy.com/
 +
 +
<!-- Please leave this at the bottom -->
 +
[[Category:Types of Glass]]

Latest revision as of 10:03, 18 February 2011

CIM stands for Creation Is Messy. They are suppliers of glass which hs a CoE of 104 and is compatible with Effetre, Vetrofond, Lauscha and the other 104 glasses. The messy colour pallettes are being extended regularly with new shades. They also produce a range of CoE 96 glass called Messy 96. Messy colour 104 and Messy 96 are not compatible.

Occasionally CiM produce a pull of glass that does not conform exactly to their colour specifications or one that is created for a test run. These occasional odd lots of glass are labled as "Messy Uniques."

Creation in Messy 104 colours and stock numbers

Information on the working properties of CiM glass is a research project by members of the Frit-Happens community in the form of a prize competition Frit-Happens CiM Competition Thread The information below has been collated by Jolene Wolfe kitzbitz art glass and is intended as a guide only.

CiM 104

Stock numbers are preceded with 511.

Stock Number Colour Properties Other Info Reactions
109 bordello intense translucent deep red
128 sangre striking colour opaque red no brown reaction with fine silver
149 lipstick opaque red brown (brick)
223 pumpkin opaque light orange
229 clockwork intense striking colour - stiff glass deep orange becomes more opaque in a reduction flame
241 creamsicle not a spreading colour opaque orange
277 phoenix striking colour Orange
346 ghee strikes from light yellow to shades of caramel semi opaque light yellow
351 stoneground works well in slightly reducing flame of a HH - reduction colour is orangy opaque light brown reacts with fine silver - reacts with ivory
402 celadon not a spreading colour opaque turquoise reacts with ivory - little reaction with fine silver
413 peacock green shocky - anneal from hot - works well in slightly reducing flame of a HH translucent light green
430 elphaba not a spreading colour - reduces to brown tones - Can appear striated opaque light green
448 dirty martini perfectly complimented by Reichenbach antique clear opaque pale green lace reaction with nero intenso - fumed easily by by silver glass and SiS and reacts butifully with fine silver leaf
449 kryptonite striking - does not work well in slightly reducing flame of a HH semi opaque light green does not react strongly with silver glass
475 commando opaque green
476 olive opaque green
478 oz vibrant trans green
479 soylent opaque green
481 splitpea heavy natural striations within this colour opaque green
482 mojito light trans green
483 slytherin very intensely saturated colour dark trans green
487 poison apple vibrant opal green
492 sherwood opaque forest green
497 appletini transparent bottle green
499 rainforest greenish teal opal
500 azure transparent blue
505 french blue has some striation opaque bright blue etches beautifully - reacts with ivory
508 leaky pen Intense colour - work high in flame as may pit - works well in slightly reducing flame of a HH - spreading colour - takes on a metalic hue when reduced - stiff glass - takes longer to etch semi translucent dark blue looks black over rubiono oro
512 halong bay shocky - anneal from hot - works well in slightly reducing flame of a HH opal light blue
519 glacier light striations within this beautiful opaque light blue
531 lapis works well in slightly reducing flame of a HH - reduces to a metalic sheen dark opaque purple blue
543 sapphire may pit if heated too quickly transparent medium blue
547 electric avenue works well in slightly reducing flame of a HH opal medium blue brown reaction with fine silver - when heavily reduced goes deep terracotta - reacts with ivory
550 chalcedony opal light blue has a light reaction with fine silver
562 ming opal deep blue coulour opacifies the longer it is worked
563 pulsar may pit if heated too quickly transparent medium blue reacts with ivory
568 freman opaque sky blue reacts with silver - reacts with ivory
569 smurfy opaque turquoise reacts with ivory
570 grumpy bear some striation opaque periwinkle
571 cornflower some striation opaque periwinkle blue
586 mermaid some striation opaque teal
589 zachary opaque baby blue
590 great bluedini intense trasparent teal
598 atlantis bluish teal opal
618 simply berry semi opaque light purple superheat with nero intenso stringer for "lace" effect - does not react as a base for silver glass
632 thai orchid intesne colour - some striation - works well in slightly reducing flame of a HH opaque violet does not react with silver glass or SIS - spreads when superheated over a softer opaque base
645 heffalump colour appears to "shift" in different lighting conditions - looks lovely coated with 00 lead crystal frit (sugared) opaque light lavender brown reaction with fine silver
652 count von count colour appears to "shift" in different lighting conditions transparent light purple/blue
653 larkspur colour appears to "shift" in different lighting conditions transparent pale purple/blue Does not lace with nero intenso
654 grape ape works well in slightly reducing flame of a HH - some striation opaque medium purple does not react with silver glass - reacts with Kugler 104 green - can "swallow" stringer - reacts with plum - reacts with copper colours
655 eggplant saturated and intense - spreading colour - works well in slightly reducing flame of a HH - striking colour opaque dark purple
658 plum works well in slightly reducing flame of a HH - Looks beautiful encased in clear - spreading colour - striking colour opal light purple reacts with ivory - not fumed by gold leaf - can "swallow" stringer - reacts with grape ape - reacts with copper colours
660 crocus Looks beautiful encased in clear semi opaque light purple
661 evil queen opaque deep purple
667 poi some striation opaque dark lilac gray
701 ginger can be shocky opaque light neutral pink less reactive than ivory
703 butter pecan opaque pale pink less reactive than ivory - reacts with fine silver foil - reacts with celadon
717 khaki works well in slightly reducing flame of a HH opaque neutral gray reacts with fine silver
722 canyon de chelly works well in slightly reducing flame of a HH - heavy striation - striking colour opaque silver light brown no lacing with nero intenso - looks great with raku
742 sepia colour appears to "shift" in different lighting conditions - work cool transparent pale pink/amber Does not lace with nero intenso - no fuming with silver glass - very effective with SiS - look nice etched
780 maple trans mid brown
788 mink opal chocolate browm
806 cirrus striking colour - shocky - anneal from hot - does not etch - works well in slightly reducing flame of a HH semi opaque white reduces to yellow/brown - Dots of leaky Pen and Reichenbach gold violet "pool" when melted in to cirrus - becomes more opaque the longer you work it in the flame - can be fumed by silver
820 hades dots crisp melted down over Effetre white - dots bleed into CiM peace - works well in slightly reducing flame of a HH opaque intense black - even as stringer reacts with ivory and opal yellow - laces as stringer over some base glasses including Effetre coral when superheated - fumes to irridescent green/blue with fine silver - reacts with palladium.
834 clear work cool transparent clear
835 peace saturated colour shimmering opaque white
859 marshmallow Looks beautiful encased in clear semi opaque white
872 tuxedo grey based opaque black effetre white stringer breaks up organically over a tuxedo base
874 adamantium opaque dark grey
885 gunmetal soft glass black glass that tends towards silver/pewter in a neutral to oxygen rich flame
904 gelly's sty likes to be worked hot opaque light pink
907 rose quartz likes to be worked hot (may devit in a cooler flame ) - looks lovely coated with 00 lead crystal frit (sugared)- striking colour semi opaque light pink brown reaction with fine silver
915 pink champagne colour appears to "shift" in different lighting conditions translucent light pink brownish tint when used to encase white
921 blush trans pale pink
926 cranberry pink spreading colour - makes beautiful vivid pink when encased over white/dark fuchsia over ivory - burns less easily than Effetre Rubino Oro semi opaque rich dark gold pink - available in two distinct shades (511926-1 light & 511926-2 dark) very reactive (dirty martini, lapis)
957 desert pink works well in slightly reducing flame of a HH opaque pale pink Fumed easily by silver glass

CiM Limited Runs

Stock Number Colour Properties Other Info Reactions
511484 algae transparent greyish green
511656 black currant very dark purple (nearly black)
511765 chai light opaque brown
511773 tamarind opaque mid chocolate brown
511795 adobe adobe brown opaque
511891 hippo opaque grey
511864 charcoal very dark trans grey
511893 african gray keeps cat's-eye sheen, good base for silver opaque mid grey
511896 oliphaunt good base for silver opaque grey, blueish not brown
511939 - cored cane cranberry pink and gelly's sty cored cane, heart shaped cranberry encased with gelly's sty streaky pink when worked
511938 - cored cane peace and gelly's sty cored cane, heart shaped peace encased with gelly's sty streaky pink and red when worked
511994 razzleberry hot pink

CiM Uniques

Stock Number Colour Properties Other Info Reactions
511128-1 sangre darker than regular sangre
511140-1 lipstick lighter thank regular lipstick
511140-3 lipstick lighter than 5111140-1
511223-3 Pumpkin not a spreading colour lighter than regular pumpkin
511223-3 pumpkin translucent burnt orange
511333 sunshine never went in to full production soft buttery yellow
511351-1 stone ground lighter than regular
511413-2 peacock green slightly blueish compared to regular
511413-3 peacock green more saturated than 511413-2
511427 tabby gray never went in to full production - looks great with SiS silver gray
511430-1 elphaba very similar to regular
511430-2 elphaba petroleum green
511430-3 elphaba darker than regular
511449-1 kryptonite turns opaque more quickly than regular
511531-1 lapis more purple than blue
511618-1 simply berry lighter than regular
511618-2 simply berry darker than regular
511644 dusk never went in to full production - colour shifts under different lighting blue gray shade looks a more neutral gray when used to encase white
511656 blackcurrant almost black when used on its own very dark purple
511701-1 ginger lighter than regular
511703-3 butter pecan darker than regular
511703-3 butter pecan more yellow than regular
511742-1 sepia more amber than regular
511742-2 sepia melt came out blue
511806-1 cirrus striking colour strikes to opaque more easily than regular
511806-2 cirrus striking colour slight blue tint
511904-1 gelly's sty less saturated than regular
511957-1 desert pink brighter than regular
511957-2 desert pink peachier / more brown than regular

Two batch annealing schedules for CiM

525 (Celsius) annealing schedule for batch annealing

Ramp up         0-150  degrees       1 hour     
                   150-315  degrees    1 hour   
                   315-425  degrees    1 hour   
                   425-525 degrees     1 hour
                   Held at 525 for 30 minutes
Ramp down     525-425 degrees     2 hours
                   425-370  degrees    1 hour 
                   370-315  degrees    1 hour
                   315-205 degrees     1 hour
Turn off kiln and remove beads the next morning.

555 (Celsius) annealing schedule for batch annealing

Ramp up         0-150 degrees         1 hour
                   150-315 degrees      1 hour 
                   315-425 degrees      45 minutes
                   425-510  degrees     45 minutes
                   510-555  degrees     45 minutes
                   Held at 555 for 30 minutes
Ramp down     555-510 degrees       1 hour
                   510-455 degrees       1 hour
                   455-400 degrees       1 hour
                   400-290 degrees       1 hour
                   290-230 degrees       1 hour
Turn off kiln and remove beads in the morning.

Information researched by CiM tester Lorraine Chandler

Further information

Visit their website for more information: http://www.creationismessy.com/