Line 421: Line 421:
|moon rock
|moon rock
| striking
| striking
| strikes from brick red to purplish coral
| strikes from brick red to purplish coral
|-
|-
|1906  
|1906  
Line 451: Line 451:
|Transparent amber (streaky amber)
|Transparent amber (streaky amber)
|
|
| reacts with silver glass - reacts with ivory
| reacts with silver glass - reacts with ivory
|-
|-
|1919  
|1919  
|pale ivory
|pale ivory
|
|
| reacts with fine silver to produce organic effects
| reacts with fine silver to produce organic effects
|-
|-
|1922  
|1922  
Line 481: Line 481:
|river rock (brie)(avocado)
|river rock (brie)(avocado)
|
|
| reacts with fine silver to produce organic effects
| reacts with fine silver to produce organic effects
|-
|-
|1932  
|1932  
Line 515: Line 515:
|1943  
|1943  
|orange sherbert  
|orange sherbert  
| also called free range salmon pink
| aka. free range salmon pink
|  reacts with silver glass  
|  reacts with silver glass  
|-
|-
Line 556: Line 556:
|lemon meringue
|lemon meringue
|
|
|reacts with Effetre copper green
| reacts with Effetre copper green
|-
|-
|1951  
|1951  
Line 733: Line 733:
|  reacts with fine silver and silver glass  
|  reacts with fine silver and silver glass  
|-
|-
|1995
|jupiter
|
|  reacts with fine silver and silver glass
|-
|1996
|bloody mary
|
|  reacts with fine silver and silver glass
|=
|1997
|painted desert
| striking
| 
|-
|1998
|rhubarb
|
|  reacts with fine silver and ivory glass
|-
|1999
|petrified wood
|
|  reacts with fine silver and ivory glass
|}
|}

Revision as of 21:40, 14 November 2008

Vetrofond glass is manufactured in Italy. Many stockists of Vetrofond glass rods use their own colour descriptions and stock numbers. The last 4 digits used by any stockist for their stock numbers will refer to the Vetrofond factory stock number.

Vetrofond colours and stock numbers

Transparent

Stock Number Colour Properties Reactions
1004 clear colours appear lighter encased in clear
1005 crystal clear good for encasing silver glass
1008 yellow
1012 light topaz
1014 topaz reacts with silver glass - reacts with silver to produce organic effects
1020 light grass green reacts with silver glass
1022 grass green
1024 dark grass green
1026 teal
1028 light emerald green
1030 emerald green
1034 light aquamarine
1036 aquamarine (aqua)
1038 pale aquamarine (light aqua)
1040 light purple
1042 purple
1044 dark purple
1048 grey
1052 light blue
1054 blue
1058 intense blue
1060 cobalt blue
1064 black
1068 pink
1069 electric yellow striking
1072 orange striking
1076 red
1080 pale lavender
1082 lavender blue (alexandrite)
1084 light brown
1086 medium brown
1088 dark brown

Opaque/pastels

Stock Number Colour Properties Reactions
1204 white
1206 anice white
1208 silk white
1212 pea green
1214 nile green
1216 grass green
1218 dark grass green
1220 periwinkle
1224 light sky blue
1228 dark sky blue
1232 turquoise
1236 dark turquoise
1240 light lapis blue
1242 lapis blue
1246 cobalt blue
1248 light grey
1250 medium grey
1255 flower pink
1262 dark ivory
1264 light ivory
1268 pearl grey
1272 violet


Specials

Stock Number Colour Properties Reactions
1408 medium yellow
1412 dark lemon
1420 coral
1424 carrot red
1428 light red
1432 medium red
1438 red purple
1444 light brown
448 dark brown
1456 gold pink
1460 yellow ocher (wasabi)

Odd lots

Stock Number Colour Properties Reactions
1801 cosmic storm reacts with silver glass - bleeds in to ivory glass
1802 apricot jam
1803 candy corn
1804 tomato soup
1805 orange dreamsicle Reacts with [EDP]
1806 smoke rings semi-transparent
1807 frog pond
1808 swamp moss
1809 jungle twilight
1810 lemongrass semi-transparent reacts with iris gold frit
1811 moon rock striking strikes from brick red to purplish coral
1906 chardonnay
1909 transparent green odd
1910 transparent yellow odd
1911 silk white (opal white)
1912 olive green pastel
1917 Transparent amber (streaky amber) reacts with silver glass - reacts with ivory
1919 pale ivory reacts with fine silver to produce organic effects
1922 transparent sage green
1925 transparent pale blue
1926 sea green (seafoam)
1927 ocean green
1931 river rock (brie)(avocado) reacts with fine silver to produce organic effects
1932 fish pink
1933 pink no.3
1934 pink flower
1937 arancio perfecto
1938 pale aqua streaky
1939 intense tangerine
1943 orange sherbert aka. free range salmon pink reacts with silver glass
1940 italian marble
1941 pineapple yellow
1942 watermelon (poppy) reacts with silver glass - reacts with ivory and fine silver
1944 tangerine
1945 new white (custard)
1946 sunshine 1947 yellow ice (lemon ice)(belgian lace)
1948 banana cream
1949 lemon meringue reacts with Effetre copper green
1951 transparent candy apple red
1952 violet odd (purplicious) reacts with fine silver and also ivory to produce organic effects
1954 cool white (odd cotton) reacts with fine silver
1955 seashell swirl reacts with fine silver and ivory
1957 orange punch
1958 pyjama blue
1960 light pink
1961 carrot red this glass contains sparkles
1963 green tepenade
1964 pale avocado
1965 olive green
1966 dark olive green
1967 quartz grey
1968 slate blue
1969 pearl grey
1970 transparent streaky sapphire
1975 midnight blue black rod with a blue core
1976 key lime green
1977 parrot green
1978 transparent crystal green striking strikes to neon yellow
1980 light streaky brown
1981 streaky brown
1982 dark streaky brown
1983 pale ocean blue
1984 pale moss agate reacts with silver glass
1985 moss agate
1986 lichen reacts with fine silver and ivory
1987 dark lichen reacts with fine silver and ivory
1988 pale crystal green
1989 transparent odd topaz reacts with silver glass
1990 honey crunch reacts with fine silver and silver glass
1991 marbled avocado reacts with fine silver and silver glass
1992 banana
1993 sweet lime (red jasper) reacts with fine silver and silver glass
1994 strawberry sweet (dark red jasper) reacts with fine silver and silver glass
1995 jupiter reacts with fine silver and silver glass
1996 bloody mary reacts with fine silver and silver glass = 1997 painted desert striking
1998 rhubarb reacts with fine silver and ivory glass
1999 petrified wood reacts with fine silver and ivory glass